Catalogue of resistive facings
Key references: Vér & Beranek 2006
Each catalogue has a page of its own: choose another one here and open it, or narrow the rows of this one by name and by the table that printed them.
Twenty-nine thin resistive facings, the wire meshes, glass cloths and sintered metal sheets that go over a porous absorber or across the mouth of a cavity, each with the flow resistance of unit area of it. That is the thing this table is most likely to be misread for. The porous catalogue holds a flow resistivity, per metre of the bulk material it describes; a facing is a sheet with no thickness worth dividing by, so what is measured on it is a resistance in pascal seconds per metre, and the two quantities are a thickness apart. Multiplying one of these rows by a thickness gives a number nobody measured.
Two of the three tables print that resistance twice, once as the page’s N s/m³ and once as a multiple of the characteristic impedance of air, and neither says what it took the impedance to be. Both columns are kept as printed rather than one being recomputed from the other, because dividing them gives the impedance back: the wire meshes imply 407 to 421 Pa s/m and the sintered sheets 400, except for the one block that implies 397.7, which is a property of the page and not of any facing. The sintered sheets are also the only rows with a nonlinearity factor, the ratio of the resistances measured at face velocities of 500 and 20 cm/s, and they run from 1.8 to 5: a facing at 1 would be the linear one the rest of this library assumes. The others are named by what a weaver would call them, a wire count or a weave, and the search matches a bare number because that is what a glass cloth is called.
Italic is a value this library worked out; a dotted underline is a cell that is not a plain number, and what it is reads on the cell; an asterisk is a note the page made about the row. Click a mark to read it, or give the table focus and press Enter to walk the marks with the arrow keys.
| Facing | Weave | Specific flow resistance Pa·s/m | Normalized flow resistance | Wires per centimetre 1/cm | Wire diameter µm | Thickness mm | Mass per unit area kg/m² | Surface density g/m² | Nonlinearity factor | Source |
|---|---|---|---|---|---|---|---|---|---|---|
| 12 | 5.7 | 0.014 | 12 | 330 | 1.6 | Vér & Beranek 2e TABLE 8.5, PDF page 266 (printed p. 262) | ||||
| 20 | 5.9 | 0.014 | 20 | 220 | 1.2 | Vér & Beranek 2e TABLE 8.5, PDF page 266 (printed p. 262) | ||||
| 40 | 9 | 0.022 | 40 | 115 | 0.63 | Vér & Beranek 2e TABLE 8.5, PDF page 266 (printed p. 262) | ||||
| 47 | 13.5 | 0.033 | 47 | 90 | 0.48 | Vér & Beranek 2e TABLE 8.5, PDF page 266 (printed p. 262) | ||||
| 80 The page prints this mass twice, 0.31 kg/m2 and 0.63 lb/ft2, and 0.63 lb/ft2 is 3.08 kg/m2, ten times the first. The defective cell is the pound one, the restatement, which this catalogue does not hold; the row serves the 0.31 kg/m2 that the column above it and the weave of the mesh both support. See docs/ERRATA.md. | 24.6 | 0.06 | 80 | 57 | 0.31 | Vér & Beranek 2e TABLE 8.5, PDF page 266 (printed p. 262) | ||||
| 120 The page prints this surface density twice, 3.16 oz/yd2 and 96 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.6 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 60 × 58 | 300 | 96 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 126 The page prints this surface density twice, 5.37 oz/yd2 and 164 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.0 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 34 × 32 | 45 | 164 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 138 The page prints this surface density twice, 6.70 oz/yd2 and 204 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.4 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 64 × 60 | 2 200 | 204 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 181 The page prints this surface density twice, 8.90 oz/yd2 and 272 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 10.9 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 57 × 54 | 380 | 272 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1044 The page prints this surface density twice, 19.2 oz/yd2 and 585 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.3 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 14 × 14 | 36 | 585 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1544 The page prints this surface density twice, 17.7 oz/yd2 and 535 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 12.2 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 14 × 14 | 19 | 535 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 3862 The page prints this surface density twice, 12.3 oz/yd2 and 375 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.2 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 20 × 38 | 350 | 375 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1658 The page prints this surface density twice, 1.87 oz/yd2 and 57 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.2 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 24 × 24 | 10 | 57 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1562 The page prints this surface density twice, 1.94 oz/yd2 and 59 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.5 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 30 × 16 | < 5 | 59 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1500 The page prints this surface density twice, 9.60 oz/yd2 and 293 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.1 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 16 × 14 | 13 | 293 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1582 The page prints this surface density twice, 14.5 oz/yd2 and 442 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.2 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 60 × 56 | 400 | 442 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1584 The page prints this surface density twice, 24.6 oz/yd2 and 750 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.2 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 42 × 36 | 200 | 750 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| 1589 The page prints this surface density twice, 12.0 oz/yd2 and 366 g/m2, and one ounce per square yard is 33.906 grams per square metre to three decimals, by the exact definitions of the ounce and the yard, so the two printings are 11.2 per cent apart. The whole column is, by the same factor; the page does not say which of its two columns carries it, so this row holds the g/m2 as printed and docs/ERRATA.md argues the pair. Footnote a: “Averaged over a large sample.” | 13 × 12 | 11 | 366 | Vér & Beranek 2e TABLE 8.6, PDF page 267 (printed p. 263) | ||||||
| FM 125 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 100 | 0.25 | 1 | 3.9 | 3.6 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 127 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 100 | 0.25 | 0.76 | 3.3 | 5 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 185 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 100 | 0.25 | 0.5 | 2 | 2.6 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| 347-10-20-AC3A-A Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 100 | 0.25 | 0.5 | 1.32 | 2 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| 347-10-30-AC3A-A Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 100 | 0.25 | 0.76 | 1.1 | 2 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 802 Hastelloy X, the one material footnote a excepts. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 100 | 0.25 | 0.5 | 1.3 | 2 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 134 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 350 | 0.88 | 0.89 | 3.8 | 4.7 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 122 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 500 | 1.25 | 0.76 | 1.4 | 1.8 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 126 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 500 | 1.25 | 0.66 | 3.7 | 3.6 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| FM 190 Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 500 | 1.25 | 0.41 | 2 | 3.3 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) | ||||
| 347-50-30-AC3A-A Type 347 stainless steel, per footnote a. The flow resistance is for air at 70°F, per the column spanner, “Specific Flow Resistance Air, 70°F”. | 500 | 1.25 | 0.76 | 1.4 | 2 | Vér & Beranek 2e TABLE 8.7, PDF page 267 (printed p. 263) |
References
Section titled “References”- Vér, I. L., & Beranek, L. L. (2006). Noise and vibration control engineering: Principles and applications (2nd ed.). Wiley. https://doi.org/10.1002/9780470172568 Tables 8.5 to 8.7: the source of the rows of the catalogue of resistive facings that cite it.